Analysis of plate corrosion and rubber mat aging in plate heat exchanger

Plate heat exchanger as a compact and efficient heat exchange equipment, although its development has been nearly a hundred years old, and in some sectors (such as food, pharmaceutical, chlor-alkali, etc. Industry) has a wide range of applications, but due to its lack of temperature, pressure, corrosion resistance and other capabilities, it limits its application. In the evaporation section of the ion membrane workshop of a factory in our company, two MB100 plate heat exchangers are used to cool the lye in parallel. The hot fluid inlet medium of the heat exchanger is an alkali solution (containing a small amount of salt) with a temperature above 85 °C, and is exported. The temperature is about 50 °C. The plate heat exchanger is made of 304 stainless steel plate, which suppresses the adult-shaped 0.6mm thick corrugated plate, and is composed of a labyrinth-shaped fluid passage with a reversed left and right herringbone groove. After two years of use, the plate heat exchanger leaked, and the plate heat exchanger was prevented from leaking after one month. The following is a brief analysis of the reasons for the failure of the plate heat exchanger.
Sealing failure
Seam gasket material
The detachable plate heat exchanger leaks when used, and the failure of the gasket material is an important factor in addition to sheet corrosion. There are mainly the following ways: 1 When the rubber gasket material is in contact with the fluid, when a fluid component penetrates into the rubber, sometimes the soluble substance can be extracted, resulting in swelling of the rubber gasket; 2 the presence of halogen and ozone The effect is to soften the gasket or cause stress corrosion cracking. 3 Under certain conditions, especially at high temperatures, the elastic material will decompose and release chemicals, which themselves will corrode the sheet material, such as FPM rubber will release oxygen. After disassembling the plate heat exchanger, it was found that the cold fluid end surface of the plate was bright, a small amount of black scale was locally, the number of corrosion pits was small and did not penetrate, and there was black deposit in the corrosion pit, so it can be inferred as a gasket. Piece of corrosion exists.
Fluid pressure
Removable plate heat exchangers leak when used within the rated working pressure, except for the quality factors in the manufacturing assembly, mainly in the system The water hammer and the air hammer are related to the abnormal impact load, which is a phenomenon that is not easily observed during use. The instantaneous pressure peak caused by the impact is often 1-3 times higher than the normal working pressure, causing the rubber gasket installed in the plate heat exchanger to shift, resulting in seal failure. Since the heat transfer element of the device is made of a stainless steel sheet (thickness of 0.5-1.0 mm), the sealing rigidity is relatively poor and the sealing perimeter is long, so the impact pressure resistance is much lower than that of the shell-and-tube heat exchanger. The abnormal impact of the plate heat exchanger can be judged according to the equipment for providing the conveying medium. When the alkali pump for transporting the alkali liquid to the plate heat exchanger is repaired, it is found that there is a small amount of honeycomb in the pump casing, indicating that the pump is running. There is cavitation; at the same time, due to the leakage around the previous plate, it can be inferred that the change of fluid pressure is also a possible factor of leakage.
Temperature
A sharp change in temperature can also cause seal failure. When the temperature changes too fast, the coefficient of linear expansion of the rubber gasket does not match the elastic deformation amount and the sealing pre-tightening force, so that the sealing pre-tightening force is lowered, and the pressure bearing capacity of the device is lower than the rated design pressure.
From the working conditions of the plate heat exchanger, the temperature has little effect on it, so it can be excluded.
Corrosion
The corrosion of plate heat exchangers mainly refers to the corrosion of the plates. Plate heat exchangers are mostly made of stainless steel sheets. Although stainless steel has good corrosion resistance, it will cause uniform or partial corrosion of the stainless steel sheets after the passivation film is destroyed. The corrosion phenomenon exhibited by the plate heat exchanger is mostly stress corrosion caused by Cl-, which often occurs at the bottom of the sealing groove of the plate and the bottom of the scale after the formation of dirt. The main reason is that: 1 stainless steel plate is mechanically cold pressed. Inevitably, a certain amount of surface residual stress remains inevitably. For a stainless steel sheet containing no molybdenum element, the elimination of surface residual stress is difficult. After the two sheets are assembled, a multi-slit structure is formed, and the corrugated top ends of the adjacent sheets cross each other to form a large number of contacts. There will be gaps in the cross-contacts, and the medium in the gaps will not flow smoothly, so that there is a difference in the concentration of oxygen inside and outside the gap, causing crevice corrosion. 3 When the dirt on the surface of the plate is serious, the corrosion elements (Cl, S, etc.) in the medium may adhere to the dirt in a large amount and be enriched in the gap of the bottom. 4 The harmful elements in the bottom of the sealing groove are often the precipitation of Cl in the adhesive due to temperature rise. For example, the neoprene series of adhesives and compressed asbestos mats (containing CaCl2) tend to form ClCl and H+ in the water and steam conditions, resulting in severe stress corrosion at the bottom of the groove. Cracking. When the unpacked sheets were inspected, it was found that most of the sheets at the inlet of the hot fluid side had cracks, and there was a thick layer of dark brown deposit before the cleaning; on the hot-fluid inlet side of the sheet, the top of the herringbone corrugated, adjacent The contacts on the top of the corrugated corrugations have point-like surface damage and corrosion spots, surrounded by dark brown deposits. Perforation corrosion occurs in 1 or 2 places on each plate, and is located at the cross-over contacts of the corrugated tip near the hot fluid inlet side, and the local area is corroded pitting and pit. The crack on the side of the hot fluid in the perforated corrosion pit is obvious, and most of the corrosion is in the shape of a slit, and most of it has penetrated. Therefore, it can be judged that the corrosion condition of the plate heat exchanger is a comprehensive reaction of various factors.
Analysis and Discussion
According to the above analysis and test results, the heat exchanger plate failure is mainly corrosion failure,
The heat exchanger uses EPDM as a gasket. Due to the high inlet temperature and the pressing force, the S element in the pad is in contact with the plate. Produces a certain sulfide that promotes the occurrence and expansion of corrosion.
The heat exchanger is composed of a plurality of plates alternately arranged and pressed together, and the corrugated top ends of adjacent plates cross each other to form a large number of contacts. There will be gaps on the cross-contacts, and the medium in the gaps will not flow or flow poorly, resulting in a difference in the concentration of oxygen inside and outside the gap, causing crevice corrosion, causing certain areas in the gap to preferentially corrode and dissolve, which is in contact The main cause of perforation corrosion at the point.
contains a small amount of sodium chloride in the lye, so that the plate contains a higher concentration of Cl- ions in the gap, due to its strong penetrating ability, damage It even penetrates the surface passivation film, so that the base metal directly contacts the medium, causing corrosion to dissolve; the presence of the S element may generate some sulfide, which promotes the occurrence and expansion of corrosion.
The heat exchanger herringbone corrugated sheet is stamped and formed into a large amount of martensite, and the crystal is dispersed into fine carbides. Stainless steel has reduced corrosion resistance. The residual stress after deformation, together with the tightening force applied during the assembly of the sheet, causes large stresses at the top of the corrugation, promotes intergranular corrosion, and causes cracks to propagate along the crystal.
In the operating system, when the heat exchanger is subjected to an abnormal impact exceeding the rated load, the displacement of the gasket is liable to occur and leakage is caused.
The quality and service life of plate heat exchangers depends to a large extent on the quality and service life of the gasket. For large logarithmic heat exchangers, the plates are generally not damaged, and the gaskets are prone to aging and cause leakage, so the quality of the gasket determines the quality and service life of the heat exchanger.  
2019/05/11 08:34:07 4230 Click

美人巨大的荫蒂BBW-国产午夜在线精品三级a-一级a一片久久久精品网-亚洲毛茸茸的mm | 亚洲日本精品-伊人网,中文字幕-大地影院mv在线观看高清-女人自蔚免费一级看片 | www.干456-欧美色图一区二区三区-一级AV在线-妃光莉AV亚洲一区二区 | 东北熟女自慰-少妇厨房愉情理伦bd在线观看-亚洲精品视频福利网-另类裸女色情毛片 | 操东北妓女-大桥未久黑人mibd445封面-亚洲 女同志 年轻 热 free-V本道V视频 | 123网址色伊人-伊人干干干-国产 老头 视频-国产美女裸体无遮挡免费视频 | www.绿帽av-日韩欧美精品一中文字幕-伊人久色-亚洲综合女教师旗袍av | baoyu135精品国产尤物-精品1区2区午夜精品 国产乱人伦偷精品视频免下载-26uuu性欧美-国产精品一区二区av影院蜜芽 | 1769色欲视频-试看免费h-已婚少妇口述与入室小偷偷情-一本道综合免费视频 | 中文字幕色情日本亚洲A-99re热免费精品视频观看-久久久久久久97-另类BwBWBwBWBW视频 | 亚洲人成电影福利在线播放-大香蕉丝袜诱惑-日韩精品成人a在线观看-搡老女人老91妇女老熟女 | 男女草逼网站-欧美成人精品第一区二区三区-悠悠裸体女-盗摄国产女洗澡79胴体 | 一本加勒比HEYZO爆-4k在线观看完整版 午夜看一级特黄a大片-顶尖亚洲黄色-性――交――性――乱老妇 | 欧美一区二区抠屄视频-北条麻妃欧美激情-翔田千里一区二区免费-国产中文字幕撸吧 | 舒琪45分兔费毛片-欧美激情日翰无码一二三区-国产乱子乱xxx-japanrcep老熟妇乱子伦视频 | 欧美日韩妖精视频-伊人中文字幕-超清日韩电影在线 日本又硬又爽又黄又粗的视频-黑人借宿人妻A片 | 午夜精品女人A片爽爽免费-heyzo北条麻妃美痴女AV-巨人黑人japanese极品-又粗又深又猛又爽的A片 | 东北老熟女乱轮-性欧美1819性猛交-国产在线欧美日韩精品一区-国产精品人妻系列23p | 精品国产亚洲av麻豆狂野-大乃美女性一伦一性一伦一-97超级大尻-国产美女嘘嘘 | 亚州男男性爱网站男男性爱一级片网站-日韩一级AV在线-zzzzzxxxxx 日本人-jizz极品 | 无码人妻aⅴ一区二区三区-91捆绑91紧缚调教91-又粗又长又爽又长黄免费视频-专干ChineSe老太BBw | 人妻暴露视频3p绿帽帽-中文人妻丰满熟妇伦子伦精品-对白淫语调教-四川BBBB搡BBB搡B1 | 国产黑人一区二区三区在-一区二区三区在线 最热电视剧-一本大道黑丝视频-五十路女优 | 久久久久久精品免费宅男-伊人网伊人网-91在线精品高清免费观看-日本在线观看中文字幕无线观看 | 日批视屏-1080P神马影院在线 国产真实愉拍系列-成全视频观看免费高清第1季-婷婷色影院 | 免费观看日本-欧美视频第三页-2019年中文字字幕视频-老女人日批 自拍无码视频-东北少妇不带套对白一百度-激情成人黄色-四虎中国网站 | 蓝光电影在线观看 一个人同时接三个顾客-妃光莉AV一区二区-中文字幕日本有码视频在线-欧美成人XX720 | 国产普通话刺激视频在线播放-1080在线播放 日本高清无卡码一区二区电影 -插bbbb-久草按摩电影 | Japansex偷拍照片-白丝麻麻被c到疯狂流水-寂寞熟妇大茄子自慰-HD电影免费在线 国产亚洲视频在线观看 | 992视频一区-91女孩高跟后入-激情视频区-天天射影院 | 1080迅雷电影在线 国产欧美亚洲精品a第二页 720免费在线播放 -台湾夜av-北条麻妃被躁57分-free嫩白的12sex性自由 | 91精品人妻系列动画无码-jealousvue七十路熟女-亚洲欧美国产高清va在线播放-水嫩毛片 | 亚洲精品国产一区-4399手机在线播放韩国免费-中文字幕av无码一区电影动漫-中文熟妇亚洲视频观看 森泽佳奈A V在线观看-国产熟妇 码视频黑料-中国熟女大秀逼逼-自慰网站免费看 | 狂c亲女h高潮10次-欧美日韩精品一区二区-男女草草-北条麻妃最爽的一次 | 操女大学生-四川BBB柔BBB桑BBB-极品西川在线中出播放-熟女 人妻昭和 | 成年美女黄频视频大全免费网站-九色视频PORNY国产精品-xxxx777-一乃葵被躁120分钟视频网站 | 东北在线色情视频-嫩草影院 一二三四-www一本激情国产-超碰最新进入 | 高潮娇喘刺激连续-91Porn-jizzjizzav国产-超碰老女人-操东北女人大白屁股骚逼视频 | 野外高潮X8X8x-BDBD在线观看 日产精品一区二区-国产精品久久久久久久久免费久久国产视频一区-色橹橹AV在线翔田千里 | 爱奇艺视频视频,视频网站,高清视频,电影,电视剧,动漫,综艺,音乐-www·sao-con淫色网-亚洲伊人久久综合精品-国产精品操屄屄 | 狠狠干北条麻妃-丰满少妇黄片-国产第40页-免费看女生下面网站 |